I was asked this question by a molder who was having trouble balancing a hot runner system...

Bob
We have this new mold which is running 16 cavities in PBT. Usually we can balance the mold using the drop temperatures, but that does not seem to work on this mold. Any thoughts?

My Response
Essentially, semi-crystalline polymers with a high degree of crystallinity such as PBT and nylon are not highly affected by temperature. In such a case, you will have to adjust the gates or the hot runner system itself to balance the shear of the mold.

Additional Thoughts
Cold runner systems are the best for these materials. I know many molders who use a press-side low-RPM grinder to effectively grind up the material and re-introduce PBT back into the process.

-Andy

No TrackBacks

TrackBack URL: http://blog.traininteractive.com/mt/mt-tb.cgi/265

Leave a comment

About this Entry

This page contains a single entry by Andy Routsis published on January 16, 2012 8:55 PM.

Documentation Takes Too Long... was the previous entry in this blog.

How Much Training a Week... is the next entry in this blog.

Find recent content on the main index or look in the archives to find all content.